form
liquid
color
colorless to light yellow
pH
>10
General description
Aluminum surfaces are not receptive to most plating processes due to their tendency to form oxides rapidly.Oxide formation inhibits uniform plating, resulting in inhomogeneous deposits, poor adhesion, or no deposition at all. By first applying Zincate Electroless Immersion Zinc Plating Solution to a properly prepared aluminum surface, it is possible subsequently deposit high quality electroless nickel films.
Application
Plating onto aluminum involves a multiple step process.
1.Non-etch clean the aluminum surface for up to 5 minutes with a detergent-based cleaner. Rinse thoroughly with cascading water.
2. De-smut the surface for 10-30 seconds using an acid mixture. RTM A for plastics is a suitable agent for smut removal. Rinse again thoroughly.
3. Mild etch for 5-10 seconds in a 25% solution of Aluminum Etch Type A. Rinse again thoroughly.
4. De-smut a second time and rinse as in step 2.
5. Apply the first Zincate layer. Immerse the part in the Zincate solution for 1-2 minutes at room temperature until a gray color develops. Rinse.
6. Remove the first Zincate layer using 50% nitric acid for 30-60 seconds or until the deposit turns white. Rinse.
7. Apply a second Zincate layer for 30-60 seconds. Rinse thoroughly before applying electroless nickel to the surface.
1.Non-etch clean the aluminum surface for up to 5 minutes with a detergent-based cleaner. Rinse thoroughly with cascading water.
2. De-smut the surface for 10-30 seconds using an acid mixture. RTM A for plastics is a suitable agent for smut removal. Rinse again thoroughly.
3. Mild etch for 5-10 seconds in a 25% solution of Aluminum Etch Type A. Rinse again thoroughly.
4. De-smut a second time and rinse as in step 2.
5. Apply the first Zincate layer. Immerse the part in the Zincate solution for 1-2 minutes at room temperature until a gray color develops. Rinse.
6. Remove the first Zincate layer using 50% nitric acid for 30-60 seconds or until the deposit turns white. Rinse.
7. Apply a second Zincate layer for 30-60 seconds. Rinse thoroughly before applying electroless nickel to the surface.
signalword
Danger
hcodes
Hazard Classifications
Aquatic Chronic 3 - Eye Dam. 1 - Met. Corr. 1 - Skin Corr. 1A
存储类别
8B - Non-combustible corrosive hazardous materials
wgk
WGK 1
flash_point_f
Not applicable
flash_point_c
Not applicable